Application of sound mixing iron ore prospect briquetting process raw materials and products in the blast furnace The iron ore raw material is sintered into a sintered ore by sintering. This production process is completely burned out in the material layer, the heat energy consumption is the lowest, and the production capacity is extremely high ( 1.35-1.45 t/m2h ), which can provide the necessary amount for the blast furnace. raw material. But a large amount of debris sinter produced in this process, despite numerous studies and adopted a series of organizational measures to reduce debris made, still not completely satisfactory solution to this problem, 0 Multiple crushing and sieving of sinter is the only means of obtaining sinter with stable particle size and strength. The amount of returning from the sintering process is large (up to 50% ) and the transportation costs in the plant are increased. There is also an additional expense on the extraction and crushing of the sinter. The addition of lime to the composition of the sinter can compensate for the decline in production capacity, resulting in a capacity of 1.85 t/m2h . The use of pelleting method to make iron ore raw materials into pellets has many advantages. The main advantages are: the final particle composition is strictly in accordance with the regulations, the chemical strength is high, the crumb content is low ( 2%-5% ), no mechanical processing is required. Screened several times. Disadvantage pelletizing process is that the raw material particle size and moisture very demanding, high pelletizing the metal and energy consumption, complicated firing operations. Although the pelletizing process is widely used and the pellets have higher quality performance than the sintered ore, their share in the blast furnace charge has never exceeded 20%-50% of the iron ore charge. The main reason is that the natural repose angle and yield point of the pellet mine are low, and the optimal charging system of the blast furnace cannot be guaranteed, which will cause serious corrosion of the lining. In addition, at the beginning of the reduction, the pellets lose their mechanical strength to a greater extent than the sintered ore. In order to overcome the above disadvantages of the pellets, a method of premixing the pellets and the sinter before the furnace is adopted, but the scheme is cumbersome to implement and is practically unapplied. The further development direction of the iron ore raw material agglomeration process should be to combine the sintering method and the pelletizing method into one process, taking the length of the two and making up the short of the two, producing better than the sintered ore, and superior to Agglomerate products of pellets. At this time, the theory of sintered ore block structure proposed by E.6. Wegman can be used as the theoretical basis. According to this theory, the most robust component of the sinter is the block formed around the fuel micropowder. However, there are particles of various sizes in the fuel, and the distribution of these particles in the sintered layer is disordered, so that the size of the formed blocks is extremely different. The sinter produced in this way is unlikely to contain no large amounts of debris. In addition, the use of fuel as both a heat source and a reducing agent will contribute to the increase in hot brittleness. Due to the combination of polymorphic phenomena, a large number of stress points appear in the hot brittle material, which inevitably causes cracking. It is obvious from the above that a reasonable solution for combining the two agglomeration processes should be to strengthen the final block in the form of a very rigorously sized pellet (pellet) in the raw material state, and then to After the paving, the layer is fixed and sintered by the heat generated by the fuel. The pre-agglomeration of the sinter or its components can be considered as the first step in combining the two processes. This move will increase the production of the sintering process by 22.1% and the solid fuel consumption by 12.5% . Pre-granulation of iron concentrate with lime, due to increased layer to 500 The closest solution to the above combined process is the HPS agglomeration method developed in Japan. The specific method of the process is to pre-select the fine iron concentrate into 5 Use 5 The Ukrainian National Academy of Metallurgy developed a new process for the production of mixed agglomerated raw materials (hereinafter referred to as ГOC ) using a belt roasting machine. It is characterized by 5 From 1999 to 2000 , the ЦГOK industrial agglomeration plant produced a total of 65t of spherical pellet sinter-type mixed agglomerate ironmaking raw materials. This raw material combines the excellent metallurgical properties of sinter and pellets with new properties: 1 . ГOC is generally a sintered block composed of calcined grains, that is, the ultimate broken pieces of the sintered block, which are virtually no longer broken; 2 . Whether it is a calcined grain or a sintered block, it is a spherical particle or particle system composed of a hematite shell and a magnetite core. It has a fully open pore porosity in the macroscopic structure and has the same function as a pellet. Reducibility, does not break during reduction; 3 . In terms of cold strength (impact strength 85%-87% , wear resistance 5%-8% ), ГOC greatly exceeds traditional sinter, close to high-quality pellets with high strength in reduction; ГOC does not naturally rupture Suitable for long-term storage, flipping and transportation; 4 . In terms of physical properties (natural angle of repose) ГOC is the same as sinter; 5 . In terms of chemical composition, the FOC is the same as the pellet, but due to the hematite magnetite structure, the iron content increases by 0.5% . The smelting results of ГOC in the blast furnace of the Dnepropetrovsk Steel Company's ironmaking plant fully affirmed the application effect of ГOC . In the blast furnace charge, the ГOC content in the production of cast iron and steel pig iron is 56.5%-69.8% (average 60.5% ) and -50%, respectively . At the beginning of the trial, due to the poor raw material conditions of the coking plant, the quality of coke could not keep up. In the subsequent trials, the quality of coke was improved and the slag condition was stable. During the operation of No. 2 blast furnace, the charging system is basically stable, and KPP ↓ 1.5-2.0 has been used, and the blast parameters are rarely changed. The mixed agglomerated raw materials in each trial stage promoted the stability of the blast furnace operation and improved the technical and economic indicators of ironmaking production. Therefore, the result of such a good result is that the use of mixed agglomerated materials improves the looseness of various components of the charge, and makes the distribution on the throat section more reasonable, thereby ensuring higher utilization of airflow energy in the blast furnace. rate, German steel No. 2 BF briquetting material mixed total refining cast iron 5234t, and pig iron 4923t.
E71T flux-cored wire with a nominal component 19.5% Cr -10% Ni. The protective gas is 100% CO2. It is suitable for all-position welding with excellent technological performance, stable arc, less splashing and beautiful weld form. the weld metal has good intergranular corrosion resistance and low crack sensitivity.
Application: this product can be widely used in welding petrochemical, food machinery, medical equipment, chemical fertilizer equipment, textile machinery,
E71T Welding Wire ,E71T11 Welding Wire,E71T1 Flux Cored Wire,E71T Flux Core Wire Jiangyin Vankey Machinery Technology Co.,Ltd , https://www.jswkweldingwire.com